# Analysis and Resolution of Cold Welding Issues in 0.7mm Galvanized Sheet Welding with Short-Cycle Stud Welders

- Link: https://www.hongbaiweld.com/zh_cn/news3133.html
- Published: 2026-03-09T15:40:07+08:00
- Author: zhouhui

Short-cycle stud welding is widely adopted in thin sheet joining scenarios such 
as automotive components and home appliance enclosures due to its high welding speed
and low heat input. However, when welding 0.7mm thin galvanized sheets, cold welding
defects of studs—characterized by incomplete weld fusion and insufficient bonding
strength—are prone to occur. These defects not only compromise structural integrity
but may also lead to subsequent assembly loosening and seal failure. Combining the
characteristics of galvanized sheets and the process principle of short-cycle welding,
this paper analyzes the causes of cold welding and proposes targeted solutions for
the automotive manufacturing industry.

![](https://www.hongbaiweld.com/wp-content/uploads/2026/03/2026030907261117.png)

### I. Core Causes of Cold Welding: Galvanized Coating Interference & Heat Input Imbalance

Short-cycle stud welding achieves metallurgical bonding between studs and base metals
through instantaneous arc heating, rapid cooling, and precise heat input control.
Yet the properties of the galvanized coating on 0.7mm sheets (melting point at 419
℃, boiling point at 907℃, far lower than steel’s 1538℃) and the high thermal conductivity
of thin sheets undermine welding stability in two key aspects:

#### 1.Galvanized coating heat absorption and volatilization interference:

Under arc heating, the galvanized coating melts and volatilizes prior to the steel
sheet, generating zinc vapor. Without proper coating removal or parameter setting,
zinc vapor blocks direct contact between the arc and steel sheet, leading to insufficient
molten pool temperature and incomplete fusion—i.e., cold welding. Meanwhile, zinc
vapor is likely to cause spatter, damaging molten pool continuity.

#### 2.Heat input imbalance:

The high thermal conductivity of 0.7mm thin sheets means excessive welding current
or extended welding time can easily cause burn-through, while insufficient current
or overly short time results in inadequate melting of studs and steel sheets, failing
to form an effective fusion layer. Both scenarios trigger cold welding.

### II. Systematic Solutions: Precise Control of Pretreatment, Parameters and Processes

To resolve cold welding of studs on 0.7mm galvanized sheets for automotive production,
the core approach is to eliminate galvanized coating interference and match the 
thermal characteristics of thin sheets, implemented through three aspects: material
pretreatment, welding parameter optimization and welding process control.

Video Showcase：https://www.linkedin.com/feed/update/urn:li:activity:7435609190217412608/

(1) Galvanized Sheet Pretreatment: Eliminate Coating Interference, Strengthen Interface
Bonding Targeting the galvanized coating—the primary cause of cold welding—pretreatment
is adopted to reduce its impact on welding, with tailored methods for batch and 
single-piece production in automotive workshops: Local cleaning: For single-piece
or small-batch production, grind the welding area (diameter ≥1cm) with 80-120 mesh
sandpaper or special zinc remover to completely remove the galvanized coating and
expose fresh steel. Avoid steel wire brushes (prone to iron chip residue); clean
dust with alcohol or acetone after grinding. Overall pretreatment: For mass production
in automotive lines, adopt laser cleaning (high efficiency, no residue) or sandblasting(
suitable for large areas). This not only removes the galvanized coating but also
controls the steel sheet surface roughness at Ra≤12.5μm, enhancing the mechanical
interlocking force between studs and steel sheets.

(2) Welding Parameter Optimization: Adapt to Thin Sheet and Coating Properties, 
Strictly Control Heat Input Following the principle of low temperature and rapid
welding, adjust the core parameters (current, time, lift height) and arc initiation
parameters of short-cycle stud welding to suit 0.7mm galvanized sheets for automotive
applications:

**Core parameters: **

① Current: Refer to the formula I=(95-110)d (d = stud diameter in mm) and reduce
by an additional 10%-15% (e.g., 550-600A recommended for M6 studs) to prevent overheating;

② Time: Refer to the formula t=(4-5)d (ms) and shorten to 20-25ms (e.g., 24ms for
M6 studs) to reduce heat accumulation;

③ Lift height: Control at 1.0-1.2mm for servo welding guns to ensure stable arc 
and prevent zinc vapor from diffusing into the molten pool. Arc initiation parameters:
Retain the pilot arc (arc initiation current 30-50A, duration 20-40ms) to pre-clean
residual galvanized coating and surface oil on steel sheets, enhancing the fusion
effect of the subsequent main arc.

(3) Process Control: Full-Link Assurance, Avoid Human and Equipment Errors in Automotive
Production

Equipment calibration: Regularly verify the verticality (deviation ≤±2°) and clamping
force of welding guns to prevent arc deviation caused by loose studs. Inspect grounding
circuits to ensure grounding resistance ≤10Ω and stable current transmission—critical
for consistent welding quality in automotive mass production.

Personnel operation: Require operators to implement the “check-adjust-verify” process:
inspect the galvanized coating cleaning effect; conduct test welding before parameter
adjustment and first-piece verification for full molten pool and no backside burn-
through; inspect weld appearance (no blowholes, slag inclusions) and shear strength(
refer to GB/T 10045-2018, strength ≥80% of the base metal), in line with automotive
manufacturing quality standards.

![](https://www.hongbaiweld.com/wp-content/uploads/2026/03/2026030907311528.jpg)

### III. Effect Verification and Parameter Iteration: Data-Driven Welding Quality Assurance for Automotive Industry

After parameter adjustment, first-piece testing is required to verify the effect
for automotive production. Taking M6 studs welded at 600A and 24ms as an example,
three criteria must be met:

**Appearance:** Full stud forming, no backside burn-through and no blackening of
the galvanized coating;

**Strength:** No fracture after 90° hammer bending, shear strength ≥400MPa (compliant
with automotive industry standards);

**Stability:** Cold welding rate ≤1% for 10 consecutive welds, meeting the consistency
requirements of automotive mass production. If cold welding still occurs, fine-tune
parameters slightly (current ±20A, time ±1ms), or adopt AI vision systems such as
the YOLOv8 model by Hongbai Technology to monitor molten pool morphology in real
time and achieve closed-loop process optimization for automotive welding lines.

### Conclusion

The root causes of stud cold welding on 0.7mm galvanized sheets in automotive welding
are galvanized coating interference and heat input imbalance. The combined solution
of galvanized coating removal via pretreatment, parameter adaptation to thin sheets
and full-process strict control can effectively resolve this issue. The core is 
to precisely match the instantaneous heat input of short-cycle welding with the 
low heat resistance of galvanized sheets, ultimately achieving the dual goals of
firm bonding and no appearance damage for thin sheet welding— a key direction for
the development of high-precision, high-reliability thin sheet stud welding in the
automotive manufacturing industry.