When a stud weld is made correctly and the right materials are used, the welded joint is stronger than the stud or the base metal itself. That single fact is the whole reason the tensile test exists.
If the joint is stronger than the stud body, an axial pull should break the stud, not the weld. When the weld breaks first, something has drifted: welding parameters, surface condition, electrode wear, or a different material batch. The tensile test finds that drift before it reaches production parts.
The equipment manual states the purpose in one line: verify the bond strength between the stud and the base metal. The method is equally short — pull the stud axially until something breaks. The real work starts after the break, and it starts with one question: where did it break?
Fracture location: the only line that matters
Break outside the weld zone: the weld passed. When the fracture occurs in the stud shank or the threaded portion, away from the weld zone, the manual is unambiguous: the weld is sound. The logic is straightforward. As the axial load increases, whichever region is weaker gives way first. A fracture in the stud body means the joint’s bond strength exceeded the stud’s ultimate tensile strength. No instrument readings are needed — the fracture location is the verdict.
Break inside the weld zone: inspect, don’t scrap. When the fracture occurs in the weld zone, the manual calls for examination of the fracture surface. Note the wording. A weld-zone fracture does not automatically fail the part. It only means the bond strength did not exceed the stud body, and the fracture face must be measured before any judgment is made. This distinction gets misread on shop floors all the time. Scraping every weld-zone fracture wastes parts; waving them through without inspection is worse.

Stud Welding Joint: Weld Collar, Full Cross-Section Fusion and Heat-Affected Zone
That is the only dividing line. Inside the weld zone or outside it decides whether a specimen passes outright or moves to the next stage of judgment.
Inside the weld zone: the 20% unbonded rule
Once the fracture falls in the weld zone, one quantitative criterion applies: the unbonded area must not exceed 20% of the weld area.
In practice: on the fracture face, unbonded regions look flat, smooth, and in the original machined condition, clearly different from the rough, torn texture of the bonded area around them. Measure the flat region, divide by the total weld area, and compare against 20%. Under the limit, the specimen passes; over it, it fails.
Why 20%? Defect research offers a reference point: lack-of-fusion defects reduce tensile-shear strength by more than 30% (per GB/T 10045-2018). Unbonded area costs strength almost directly, so the limit sits between tolerating normal process variation and guaranteeing the joint still carries load.
The remaining 80% matters too. An unbonded area within the limit means the effective bonded area is still sufficient — the joint fails by tearing of the bonded region, a rough surface with visible plastic deformation, not by clean separation along the unbonded interface, which shows no deformation at all. An experienced inspector can tell the two apart at a glance, but the final call rests on the area measurement.
How many specimens: at least 3
The minimum is 3 studs per tensile test. The number comes from the structure of the standard test: visual inspection of all specimens, tensile testing of at least 3, bend testing of at least 3. A single specimen cannot distinguish a random fluctuation from a systematic problem. Three fractures outside the weld zone indicate a stable process; a weld-zone fracture among them shows whether it is an isolated case or a trend. The count stays low because the test is destructive and every specimen costs material.
Standard test vs. routine test
Two test levels exist, and confusing them is the most common execution error:
| Test type | Contents | When to run |
|---|---|---|
| Standard test | Visual inspection (all specimens) + tensile test (min. 3) + bend test (min. 3) | Before production welding starts; repeated after extensive welding, under supervision |
| Routine test | Visual inspection (all studs) + bend test (all studs) | After every change of work and after continuous welding for a period |
The routine test contains no tensile test. That is deliberate grading, not an omission. The routine test is a high-frequency self-check — quick to run, run often. The standard test is a low-frequency, full-scope verification of mechanical performance. Tensile testing sits in the standard test because it is destructive and costs more per specimen than bending.
A separate check applies in between: after every 100 studs welded (depending on material, stud diameter, and machine model), run visual and bend inspection as the minimum check scope. The welding count for a standard working test is set by the supervising engineer, subject to stud diameter, base material, and equipment model.
When a random test fails
The manual closes the loop with a three-step rule: if the number of failed studs in a random test exceeds the specified limit, find the cause of the failure, correct the welding parameters, and retest.
The order matters. Finding the cause comes first; adjusting parameters comes second. Skipping straight to parameter tweaks is guesswork — the process may pass today and fail again tomorrow for the same underlying reason, expressed differently. And retesting is mandatory. Corrected parameters alone do not return the process to production.
Preparing the test specimens
Test studs are welded onto a separate base plate smaller than 700 × 200 mm, with weld positions at equal distance from the plate edges.
Two requirements, two reasons. The test plate is prepared separately from production workpieces, so destructive testing never damages a product. And equal edge distance keeps the boundary conditions identical: a stud welded at the plate edge cools differently from one welded at the center, so the welds would not be comparable. This detail is often skipped, and it directly decides whether the three specimens can be compared against each other at all.
Visual inspection: the trigger, not the verdict
The manual defines visual inspection plainly: a rough check for major defects and an estimate of weld uniformity. When doubt remains, tensile and torque testing follow.
So tensile tests run in two ways: fixed, as part of the standard test before production welding; or targeted, as a follow-up when visual inspection raises a question. The second path is more common in daily production — an operator spots an abnormal weld appearance during patrol inspection, pulls one stud, and reads the fracture face.
Tensile and bend testing: a matched pair
The bend test is a rough check of the selected welding parameters: a specific tube bends the stud by 30°, on at least 3 studs. No cracks and no fracture in the weld zone mean the weld passed. Where the tensile test measures axial strength, the bend test measures the joint’s capacity for plastic deformation. A joint can pass tension and crack in bending, or bend cleanly and show a poor fracture location in tension. Neither test covers for the other.
One caution on the acceptance angle: the equipment manual specifies 30° for all processes, while standards research splits the requirement by process — 30° for capacitor-discharge stud welding and 60° for drawn-arc stud welding, per GB/T 2653-2008. Cite the source when you quote a figure, and don’t mix the two.
The laboratory route: GB/T 2651 criteria

Axial tensile testing evaluates the bond strength of a welded stud and helps identify potential weld defects.
A second, independent set of rules comes from standards research, and it asks different questions than the equipment manual:
- Purpose: measure the joint’s tensile strength, yield strength, and elongation.
- Specimen: a joint sample containing the stud and the workpiece, length ≥ 150 mm, threads retained.
- Method: clamped in an electronic universal tensile testing machine, loaded at ≤ 5 mm/min to fracture. Machine capacity 1000 kN, accuracy ±1%.
- Acceptance: joint tensile strength ≥ the base metal minimum, and elongation ≥ 80% of the base metal value. For a low-carbon steel base metal with ≥20% elongation, the joint must reach ≥16%. Per GB/T 2651-2008 (Tensile test method for welded joints), one published criterion requires joint strength ≥369 MPa where the low-carbon steel base metal minimum is 410 MPa.
| Dimension | Equipment manual route | Standards research route |
|---|---|---|
| Quantity judged | Fracture location | Tensile strength and elongation |
| Acceptance | Outside weld zone = pass; inside = unbonded area ≤ 20% | Strength ≥ base metal minimum; elongation ≥ 80% of base metal |
| Equipment | Pull device (optional stress gauge) | Universal tensile testing machine |
| Where it fits | On-site judgment | Laboratory verification |
The two routes do not conflict. The manual route is the fast judgment anyone on the floor can run; the standards route is the quantitative laboratory confirmation. Screen on the floor, confirm in the lab.
Why the defects matter, in numbers
Three figures from defect research explain why this test deserves attention: lack-of-fusion defects reduce tensile-shear strength by more than 30% (GB/T 10045-2018); porosity cuts fatigue life by more than 50%, with high-strength steel stud welds dropping from 106 cycles to below 105; and crack regions in high-strength steel show hardness above HV 450, indicating martensite. Strength, fatigue, and microstructure all degrade with welding defects, and the tensile test measures the most direct of the three.
The full mechanical test suite
| Test | Purpose | Key criterion | Standard |
|---|---|---|---|
| Tensile | Strength, yield strength, elongation | Joint strength ≥ base metal minimum | GB/T 2651-2008 |
| Bend | Plastic deformation capacity | No cracks at 30° (CD) / 60° (drawn-arc) | GB/T 2653-2008 |
| Impact | Impact toughness | ≥27 J at room temperature | GB/T 2650-2008 |
| 扭矩 | Resistance to twisting | Withstands 1.5× installation force without loosening | — |
The torque criterion deserves a note of its own. After stud welding, the stud usually carries a nut or a connected part, and assembly applies a tightening torque. How much torque the weld survives before loosening decides whether assembly can proceed at all — which is why the criterion is written against the installation force, not an abstract lab number.
常见问题
What does it mean if a stud weld breaks outside the weld zone?
The weld passes. A fracture in the stud shank or threaded portion, away from the weld zone, shows the joint's bond strength exceeded the stud's ultimate tensile strength, so the weld is sound.
Does a weld-zone fracture mean the part must be scrapped?
No. A weld-zone fracture only means the bond strength did not exceed the stud body; the fracture surface must be examined before any judgment is made.
What is the acceptance limit for unbonded area in a stud weld tensile test?
The unbonded area must not exceed 20% of the weld area. Measure the flat, smooth region in original machined condition on the fracture face, divide by the total weld area, and compare against 20%.
Why is the unbonded area limit set at 20%?
Defect research cited in the guidance notes lack-of-fusion defects reduce tensile-shear strength by more than 30% (per GB/T 10045-2018); the limit balances normal process variation against keeping enough bonded area to carry load.